Dopant concentration:
Nd:1.1¡«1.4at%, Ce:0.05¡«0.1at%
Orientation:
[111] within 5¡ã
Wavefront Distortion:
¡ÜLambda/8 @632.8nm
Extinction Ratio:
¡Ý28 dB
Rod Sizes:
Upon request of customer
Dimensional Tolerances:
Diameter:+0.00/-0.05mm, Length: ¡À 0.5mm
Barrel Finish:
Ground Finish: 400# Grit
Parallelism:
¡Ü15" Arc Second
Perpendicularity:
¡Ü5¡ä Arc Minute
Flatness:
¡ÜLambda/10 @632.8nm
Surface Quality:
10/5 Scratch/Dig. (per MIL-O-13830A)
Chamfer:
<0.1 mm @ 45¡ã
AR Coating Reflectivity:
¡Ü 0.25% (@1064nm)
Laser Transition
4F3/2--> 4I11/2
Laser Wavelength
1.064¦Ìm
Photon Energy
1.86¡Á10-19J@1.064¦Ìm
Emission Linewidth
4.5Å @1.064¦Ìm
Emission Cross Section(Nd1at%)
2.7~8.8¡Á10-19cm-2
Fluorescence Lifetime (Nd1at%)
230¦Ìs
Index of Refraction
1.8197@1064nm
Crystal Structure
Cubic
Lattice Parameters
12.01Å
Melting Point
1970¡æ
Moh Hardness
8.5
Density
4.56¡À0.04g/cm3
Specific Heat (0-20)
0.59J/g.cm3
Modulus of Elasticity
310GPa
Young's Modulus
3.17¡Á104Kg/mm2
Poisson Ratio
0.3(est.)
Tensile Strength
0.13~0.26GPa
Thermal Expansion Coefficient
[100]Direction:8.2¡Á10-6/¡æ(0~250¡æ)
[110]Direction:7.7¡Á10-6/¡æ(0~250¡æ)
[111]Direction:7.8¡Á10-6/¡æ(0~250¡æ)
Thermal Conductivity
14W/m/K(@20¡æ)
10.5W/m/K(@100¡æ)
Thermal Optical Coefficient (dn/dT)
7.3¡Á10-6/¡æ
Thermal Shock Resistance
790W/m
Solubility
Water:Insoluble; Common Acids:Slightly